阀门用低温钢铸件技术条件、铸件的化学成分(质量分数)_阀门标准

阀门用低温钢铸件技术条件、铸件的化学成分(质量分数)

名 称

材 料 牌 号

主要化学元素a

(%)

C Si Mn P S Ni Cr Mo Cu V
碳钢 LCA ≤0.25b ≤0.60 ≤0.70b 0.040 ≤0.045 ≤0.50c ≤0.50c ≤0.20 ≤0.30c ≤0.30c
LCB ≤0.30b ≤1.00b ≤0.20c
碳锰钢 LCC ≤0.25b ≤1.20b
碳钼钢 LC1 ≤0.25 0.50~0.80 0.45~0.65
2.5%镍钢 LC2 2.00~3.00
镍铬钼钢 LC2-1 ≤0.22 ≤0.50 0.55~0.75 2.50~3.50 1.35~1.85 0.30~0.60
3.5%镍钢 LC3 ≤0.15 ≤0.60 0.50~0.80 3.00~4.00
4.5%镍钢 LC4 4.00~5.00
9%镍钢 LC9 0.13 0.45 0.90 8.50~10.00 0.50 0.20 0.30 0.03

12.5%

铬镍钼钢

CA6NM 0.06 1.00 1.00 0.030 3.50~4.50 11.50~14.00 0.40~1.00

奥氏体

不锈钢

ZG03Cr18Ni10 0.03 1.50 0.80~2.00 8.00~12.00 17.00~20.00
ZG08Cr18Ni9 0.08 8.00~11.00
ZG12Cr18Ni9 0.12 0.045
ZG08Cr18Ni9Ti 0.08 0.040

Ti5 (C-

0.02)~

0.7

ZG12Cr18Ni9Ti 0.12 0.045
ZG08Cr18Ni12Mo2Ti 0.08 0.040 11.00~13.00 16.00~19.00 2.00~3.00
ZG12Cr18Ni12Mo2Ti 0.12 0.045
CF3 0.03 2.00 1.50 0.040 0.040 8.00~12.00 17.00~21.00
CF8 0.08 8.00~11.00 18.00~21.00
CF3M 0.03 1.50 9.00~13.00 17.00~21.00
CF8M 0.08 9.00~12.00 18.00~21.00
CF3C 2.00

NbC*8~

1.0

  a 除给出范围外均为最大值。

  b 在规定的碳含量最大值内,每降低0.01%,将允许锰含量的最大值增加0.04%,LCA的最大值含锰量为1.10%,LCB的最大值含锰量为1.28%,LCC的最大值含锰量为1.40%。

  c 规定的微量元素,这些元素的总含量为1.00%(最大值)。

 